Fused Glass Firing Schedules and Kilns: A Beginner's Guide

Laura

Pre-cut glass shapes take away the cutting, but the kiln is where your design becomes finished glass. The firing schedule decides whether your shapes keep sharp detail, melt into soft, rounded forms or crack on the way out. This guide covers the main types of firing and what to look for in a kiln.

Important: every temperature in this post is a starting point. Always follow the firing guidance from the manufacturer of your glass, and test your own kiln, because no two behave exactly alike.

First, check your glass is compatible

Fusing only works when all the glass in a piece expands and contracts at the same rate, measured as its COE (coefficient of expansion). Common systems include COE90, such as Bullseye, and COE96, such as Spectrum and Oceanside. Never mix them, and don’t mix either with float glass. Float has its own expansion and its own firing needs. Our shapes come in COE90, COE96 and float clear, so choose the same system as your base glass.

The parts of a firing programme

Most kiln controllers let you build a schedule from segments. Each segment has three settings:

  • Ramp: how fast the temperature rises or falls, usually in degrees per hour.
  • Target temperature: where that segment ends.
  • Hold (soak): how long the kiln stays there.

A full firing has four stages:

  1. Heating: a gradual rise so the glass warms evenly and doesn’t crack.
  2. Process temperature: the top temperature and hold that decide the result (tack, contour, full fuse or slump).
  3. Annealing: a hold at a lower temperature, around 480 to 520°C depending on the glass, which relieves stress inside the glass. Skipping or rushing this is the most common reason for glass cracking hours or days later.
  4. Cooling: a controlled cool through the annealing range, then a faster cool to room temperature.

The main types of firing

Firing Typical temperature What it does
Slump about 640 to 680°C (1,185 to 1,255°F) Glass sags into a mould without fusing flat pieces together.
Tack fuse about 730 to 760°C (1,345 to 1,400°F) Pieces stick together but keep their shape and texture, so cut edges and fine detail stay crisp.
Contour (rounded) fuse about 760 to 790°C (1,400 to 1,455°F) Edges soften and round, though the surface stays slightly raised.
Full fuse about 790 to 815°C (1,455 to 1,500°F) The piece melts into a flat, smooth surface with fully rounded edges.

These are typical ranges for common glass at about 6 mm thick. Thicker glass, larger pieces and different brands can all move the numbers. Firing times and temperatures are only to be used as a guide, please check with manufacturers specifications before firing.

An example of a full fuse programme

Here’s the structure of a typical full fuse schedule, to show how the segments fit together (the numbers are examples only):

  1. Heat at about 150 to 200°C per hour to about 675°C, hold 20 to 30 minutes. This warms the glass evenly.
  2. Heat as fast as your kiln allows to 790 to 815°C, hold about 10 minutes.
  3. Cool quickly to the annealing temperature (about 480 to 520°C) and hold for 30 to 60 minutes or more, depending on thickness.
  4. Cool slowly, about 40 to 80°C per hour, down to about 370°C.
  5. Cool at about 100 to 150°C per hour to room temperature, or switch off and let the kiln cool by itself.

For a tack fuse, you’d use the same structure but drop the top temperature to the tack range and shorten or remove the hold. For a slump, the top temperature drops to the slump range.

What changes your schedule

  • Thickness and layers: thicker or layered glass needs slower heating, longer anneals and longer cooling.
  • Size: large pieces need slower rates than small ones.
  • Glass type: COE90, COE96 and float each have different temperatures.
  • Your kiln: elements, size, insulation and thermocouple position all affect real temperatures.
  • The result you want: a lower temperature or shorter hold keeps more shape and detail.

Firing pre-cut shapes

  • Tack fuse keeps detail: if you want crisp animal outlines, antlers, petals or lettering, a tack fuse holds the cut edges best. A full fuse will round them off and can soften small features.
  • Small shapes lose detail first: very small shapes (under about 6 cm) may lose fine details such as feet or narrow points, even though we cut them accurately.
  • Plan for edges: if you want a smooth, finished surface, choose a contour or full fuse, but expect shapes to spread slightly.
  • Combine thicknesses carefully: uneven layers can trap air, which shows as bubbles. A slow, long hold at the lower stage (around 675°C) helps air escape.
  • Always test: fire a spare shape or small sample first to see how your kiln and glass behave.

Choosing a kiln

You don’t need a large studio to fuse. Consider:

  • Controller: choose a programmable controller that stores multi-segment schedules. A basic dial won’t give you the control you need.
  • Size: think about the biggest piece you’ll make, then allow some room. Many beginners start with a small tabletop or hobby kiln, then outgrow it.
  • Shape and loading: top-loading (lid) kilns are common for fusing. Clamshell and front-loading designs are easier to access, but check their heat distribution.
  • Element position: kilns with elements in the lid heat the glass from above, which suits fusing. Side-only elements can leave cooler spots.
  • Shelf and kiln furniture: use a kiln shelf coated with kiln wash or lined with fibre paper, so glass doesn’t stick. Kiln posts and moulds are useful extras.
  • Ventilation and location: place the kiln on a heat-resistant surface, away from walls and flammable materials, in a well-ventilated space.
  • Power supply: small kilns may run from a standard socket, but larger ones often need a dedicated circuit fitted by a qualified electrician. Check the specifications before you buy.
  • Safety: wear protective gloves and eye protection, and never open the kiln while it is hot.

Common firing problems

  • Cracking: usually incompatible glass, a short or skipped anneal, or cooling too fast.
  • Bubbles: air trapped between layers, so heat more slowly and hold longer at the lower stage.
  • Devitrification (cloudy, rough surface): often caused by holding too long at high temperature, or by dirty glass.
  • Pieces moved or slumped: the temperature was too high for the shape, so try a tack fuse.
  • Too little detail: a lower top temperature or shorter hold usually helps.

Keep a firing log

Note your glass, thickness, schedule and the result every time. Over a few firings you’ll learn what your kiln does and build a library of schedules you trust.

Ready to fuse?

Browse our pre-cut glass shapes in COE90, COE96 and float clear, check our FAQ for glass compatibility, or get in touch if you’d like a custom shape for your next project.