Why Does Fused Glass Crack? How to Diagnose and Prevent It

Laura

Opening the kiln to find a crack across a piece you spent an evening laying up is thoroughly demoralising, and the first few times it happens it feels like bad luck. It isn’t. Glass cracks for a reason, and most of the time the crack itself tells you what that reason was. Once you can read a break, you can usually stop it happening again.

This guide covers the four main causes, how to tell them apart, and what to change next time. For the firing stages and temperature ranges behind all of it, see our guide to firing schedules and kilns.

Important: always follow the firing and annealing guidance published by the manufacturer of your glass. Kilns vary enormously, and so does glass. Treat everything below as a way of working out what went wrong, not as a schedule to copy.

Start with the timing, not the crack

Before you look at the break itself, ask one question: when did it appear?

  • It was already cracked when you opened the kiln. This points to thermal shock, or to the piece sticking to the shelf or mould.
  • It cracked days or weeks later, sitting on a shelf or in a customer’s window. This is almost never thermal shock. Delayed breaks point to stress left inside the glass, which means annealing or compatibility.

That one question rules out half the possibilities before you start.

Then read the break

The shape of a crack, and the feel of its edges, are genuinely diagnostic. Run a fingertip along the break (carefully) and look at the line it takes.

What you are looking at Most likely cause
A fairly straight break running across the piece, cutting through whatever is in its way, with edges that feel slightly softened or rounded Heated too quickly
A break with sharp, clean edges that have not rounded off at all Cooled too quickly
A curved crack, often hooking round near the edge of the piece, with sharp edges Not annealed for long enough
A crack that travels around a particular shape or colour rather than straight through it Incompatible glass

The logic behind the rounded-versus-sharp distinction is worth understanding. If the glass broke early in the firing, it then sat at high temperature long enough for the new edges to soften, so they look and feel smooth. If it broke on the way down, the kiln never got hot enough afterwards to round anything off, so the edges stay sharp.

Cause 1: incompatible glass

Every glass expands and contracts at its own rate as it heats and cools. That rate is described by its COE, or coefficient of expansion. Fuse two glasses that move at different rates and they will pull against each other as they cool, locking permanent stress into the piece.

The giveaway is a crack that avoids a particular element, running around a colour or an inlaid shape as though trying to get away from it. If you see that, suspect the glass rather than the schedule.

What to do:

  • Stay within one system. COE90 with COE90, COE96 with COE96. Never mix the two, and never mix either with float glass, which has its own expansion and its own firing needs.
  • Do not trust appearance. Two sheets can look and feel identical and still be incompatible. Thickness and colour tell you nothing about COE.
  • Test anything unknown. If you have inherited glass, or scrap with no label, fire a small test strip before you commit it to a real piece. Viewed through polarised filters, stress around an incompatible inclusion shows up as a halo.
  • Be wary of very long high soaks. Holding glass at top temperature far longer than needed can shift its behaviour slightly, which is one more reason not to over-fire.

Cause 2: thermal shock

Thermal shock is what happens when one part of a piece changes temperature faster than another. The warmer part wants to expand while the cooler part does not, and the glass gives way. It is most dangerous at lower temperatures, before the glass has softened enough to relieve any of that stress itself.

Common triggers:

  • Ramping too fast on the way up, particularly through the early stages.
  • Large or thick pieces heated at a rate that would be fine for something small. Size matters as much as thickness.
  • Cold spots in the kiln. Pieces near the door, at the edge of the shelf, or shaded by kiln furniture heat differently from those in the middle.
  • Opening the kiln while it is still hot, even briefly, to have a look.
  • A cold piece going into a warm kiln for a second firing.

The fix is almost always patience: a slower ramp, and a hold partway up to let the whole piece reach the same temperature before you go on.

Cause 3: inadequate annealing

Annealing is the controlled hold and slow cool that lets stress inside the glass even out before it becomes rigid. Skip it, rush it, or cool too fast afterwards, and you get a piece that looks perfect coming out of the kiln and cracks a fortnight later.

This is the cause people most often miss, precisely because the damage is invisible at first. A delayed crack is nearly always an annealing crack.

Things that catch people out:

  • Annealing time scales with thickness. A 6mm piece and a 12mm piece need very different holds, and the difference is not small. Your glass manufacturer publishes a chart for this — use it rather than a single schedule for everything.
  • Measure the thickest point. If your piece varies in thickness, anneal for the thickest part, not the average.
  • The cool matters as much as the hold. Coming down too quickly through the annealing range undoes the hold you just did.
  • Switching the kiln off early. Letting a kiln cool naturally is fine at low temperatures, but not while the glass is still passing through its annealing range.

Cause 4: uneven thickness and tack fusing

This one deserves its own heading because it catches experienced fusers out. A flat, even piece anneals predictably. A piece with shapes sitting proud of the base does not: the glass is thick in some places and thin in others, so different parts of it pass through the annealing range at different moments.

Tack-fused work needs noticeably more care than flat work. Give it a longer soak to even out the temperature, and bring it down through the annealing range more slowly than you would a flat piece of the same overall thickness. If your usual schedule works beautifully for flat panels and keeps failing on layered designs, this is why.

The same applies to light and dark glass side by side. Dark glass absorbs heat differently, so a design that pairs black opal against clear in a thick layup is asking more of your schedule than a single-colour piece.

Other things that crack glass

Not every break is about temperature:

  • Sticking to the shelf or mould. If the glass cannot shrink freely as it cools, it will crack. Keep kiln wash fresh and evenly applied, or use fibre paper.
  • Trapped air. A bubble expanding between layers can lift and split the glass. Heat more slowly and hold longer at the lower stage so air can escape.
  • Damaged edges going in. A chip or a tiny flaw on an edge is a ready-made starting point for a crack. Check your pieces before you lay them up.
  • Sharp internal angles. Deep notches and tight inside corners concentrate stress. Softening them slightly in the design helps.
  • Handling. Glass straight out of a kiln is tougher than it looks but not invulnerable. Let it reach room temperature properly before moving it.

How to stop it happening again

  • Keep every glass system separate in your studio, and label your offcuts.
  • Fire a test piece when you try an unfamiliar glass, a new mould or a much thicker layup.
  • Slow the ramp and add a hold partway up for anything large, thick or layered.
  • Anneal for the thickest point, and double down on both soak and cool rate for tack-fused work.
  • Keep a firing log: glass, thickness, schedule, result. After a dozen firings you will know your own kiln better than any published schedule does.
  • Resist opening the kiln early. Nothing good has ever come of it.

Can you rescue a cracked piece?

Sometimes. A clean crack on a simple piece can occasionally be re-fired and healed, though you will usually need to go back up to full fuse temperature and then anneal far more generously than you did the first time. Be aware that the piece may spread as it re-melts, so the finished dimensions can change.

If the crack is large, or sits in the interior of the piece, or the edges have already rounded off in the kiln, re-firing rarely gives a result you would be happy to sell. In that case it is usually better to treat it as a test piece, work out what caused it, and make the next one properly.

Where pre-cut shapes fit in

Using pre-cut shapes removes the cutting, but it does not remove the compatibility question. Our shapes are cut in COE90, COE96 and Float Clear, and each product page lists what is available, so match the shape to the base glass you are already working with rather than to the one that looks closest.

Bear in mind too that a shape sitting on top of a base is a tack-fused layup, with everything that implies for annealing. If you are new to this, our guide to using pre-cut glass shapes covers planning and layering a design before it goes anywhere near the kiln.

Still not sure what went wrong?

If you have a break you cannot account for, we are happy to take a look. Send us a photo of the piece with a clear view of the crack, along with the glass you used and the schedule you fired, and we will tell you what we think. Our FAQ covers glass compatibility in more detail, or you can get in touch.

Browse our pre-cut glass shapes in COE90, COE96 and Float Clear, cut in the UK and shipped worldwide.